Description
>>> GebrAnw-Dental-Base-Alloy-Adorbond-PD-1.pdf <<<
Applicable scope: | Inlays, Onlays | ● |
Crowns | ● | |
Small bridges | ● | |
Large-span bridges | ● | |
Milling, cone and attachment works | ● | |
Modeling casting | ● |
Colour: | white |
Composition: | Pd | 57,80 |
(mass fraction in %) | Ru | 0,20 |
Ag | 31,00 | |
Sn | 6,00 | |
In | 5,00 |
Technical specifications: | Density in g/cm³ | 11,4 |
Vickers hardness HV 5/30 | (s)220 (n)180 (a)210 | |
Yield strength Rp0,2 in MPa | (s)550 (n)420 (a)490 | |
Elongation at break in % | (s)4 (n)10 (a)8 | |
Average linear CTE 25 – 500 °C in 10-6 K-1 | 14,9 | |
Average linear CTE 25 – 600 °C in 10-6 K-1 | 15,1 | |
Elastic modulus in GPa | 120 | |
Melting interval in °C | 1230 - 1300 |
Processing: | Preheating temp. of the casting moulds in °C | 950 |
Casting temperature in °C | 1450 | |
Crucibles | Ceramic | |
Curing | 600°C/15min |
Suitable solders: | Joints before ceramic firing | AL 1060 W |
Joints after ceramic firing | AL 750 |
1) Brief description:
s – self-curing, n – after ceramic firing, a-s – curing from s condition
a-n – curing from n condition
2) All information about cured condition is given according to the alloy:
– Oxide firing 10min/ 960°C + 4x4min/ 960°C for yellow conventional bonding alloys
– Oxide firing 10min/ 980°C + 4x4min/ 980°C for white conventional bonding alloys
– Oxide firing 10min/ 800°C + 4x4min/ 800°C for LFC-systems
Corresponding data are true under these conditions only.
3) The ceramic firing should be carried out according to the manufacturer's instructions.