Description
>> Instructions for use Download DE/EN
>> Instructions for use Download EN/FR
Multi-purpose CoCr bonding alloy for any conventional ceramic
ADORBOND® PREMIUM is a dental cobalt-based metal-ceramic alloy. ADORBOND® PREMIUM is free of nickel, cadmium, beryllium and lead and complies with EN ISO 22674 type 5 for applications where tool parts require a combination of high stiffness and yield strength, e.g. thin removable partial dentures, parts with thin cross-sections, clasps.
Composition wi | Technical specifications (normative index, condition cast/bond) | |||||
Co | % | 59,5 | Density ϱ | g - cm-3 | 8,6 | |
Cr | % | 24,8 | Vickers hardness | HV 10 | 280 | |
W | % | 5,9 | Linear coefficient of thermal expansion α 25 - 500 °C | 10-6-K-1 | 14,0 | |
Mo | % | 4,7 | ||||
Ga | % | 4,2 | Linear coefficient of thermal expansion α 20 – 600 °C | 10-6-K-1 | 14,2 | |
Fe,Si,Mn, Nb | % | < 1 | ||||
Melting interval TS - TL | °C | 1310-1405 | ||||
Casting temperature TCast | °C | 1500 | ||||
Highest recommended bonding temperature TBr,max | °C | 980 | ||||
0,2-% Yield strength Rp 0,2 | MPa | 530 | ||||
Elastic modulus E | GPa | 225 | ||||
Elongation at break A5 | % | 14 |
Carry out wax-up as usual, but avoid wall thicknesses below 0.35 mm. Guide the casting channels indirectly. For the casting channels, use round wax wires with Ø 2-2.5 mm for single crowns and Ø 2.5-3 mm for bridges. For large jobs with 4 or more units, use distribution channels (cast bars) with Ø 3.5-4 mm, and up to Ø 5 mm for solid pontics.
Phosphate-bonded crown and bridge embedding compounds are suitable. The preheating temperature is 850-900 °C, holding time at the final temperature is min. 30 minutes. Follow the manufacture’s operating instructions for the casting machine. Always use a separate ceramic crucible for ADORBOND® PREMIUM to avoid contamination by other alloys. Clean crucible after each casting. Do not overheat the alloy. Casting can be started after all cylinders are completely melted and the melt becomes uniformly bright. Always melt with the flame in the reducing zone with circular movements above of the burner. Allow muffle to cool down to hand temperature and bed out without hitting the cone.
The commercially available normal-fusing bonding ceramics for cobalt bonding alloys with a suitable coefficient of thermal expansion (CTE) can be used. Please observe the corresponding working instructions and the information provided by the ceramic manufacturer regarding the cooling rate after firing. After bedding out:
After firing the ceramic, rubberize unveneered framework parts and polish to a high gloss with a polishing paste for dental alloys or with rotating polishing tools.
Soldering before firing with the ADORBOND® CC Lot and high-temperature flux. The width of the solder gap should be 0.05-0.2 mm. Laser welding with the ADORBOND® CC laser wire.
Metal dust is harmful to your health. Use suction when handling the powder, by finishing works and blasting. Hypersensitivity to the alloy components should be taken into account. In case of suspected intolerance with certain alloy components, the product should not be used.